Methods & sources
Each study identifies its cell, boundary conditions, modeled quantities and available measurements. Results apply to the specified cell and assumptions.
LG M50 charge and lithium plating
BatterMachine’s reduced single-particle calculation represents the 5 Ah LG M50 graphite–silicon oxide and NMC811 electrodes as two spheres. Six finite volumes per sphere track lithium diffusion. A shared negative-electrode potential divides the applied current between host insertion and one-way lithium deposition. Onset is the first calculated crossing below 0 V relative to Li/Li⁺. Integrating the plating current and applying Faraday’s law gives the mass of deposited metal.
The conductivity, exchange-current functions, open-circuit potentials and cell geometry use the Chen2020 parameters. The deposition coefficient and transfer factor use the O’Kane parameterization. This browser implementation adapts the published functions to JavaScript and uses fixed electrolyte concentration, a single cell temperature and a constant external cooling conductance. The heat calculation includes ohmic loss, insertion polarization and plating polarization. The integration stops at the selected terminal voltage, the first electrode composition limit or the observation end.
Nominal SOC counts charge delivered at the terminals and may exceed 100%. The local potential and metal inventory are model predictions. The display supplies no measured inventory for a severely overcharged M50. Other chemical decomposition, electrical protection and runaway require different models. Run the M50 calculation
Electrode parameter functions adapted from PyBaMM 25.10.2, copyright 2018–2025 the PyBaMM team, BSD 3-Clause. Scientific sources include Chang-Hui Chen and colleagues (2020) and Simon E. J. O’Kane and colleagues (2022). Chen2020 implementation · O’Kane implementation · Full BSD notice
Panasonic NCR18650B forced discharge
The modeled voltage and first-order surface temperature use parameters estimated from the published 1.625 A protocol. Three time intervals were held out when fitting the coefficients. The page reports voltage errors only up to the earlier modeled or observed reporting threshold, on timestamps with measurements. The temperature panel uses its own published clock. The article’s temperature figure and method give inconsistent specimen labels, so exact correspondence between the voltage and temperature cells is uncertain. Changing the reporting threshold crops the comparison. Run the discharge study
Raghav Sai Thiagarajan, Anthony Concepción, Deepti Tewari, Judith A. Jeevarajan, Vinay Premnath and Venkat R. Subramanian. Modeling the Effect of Over-discharge Cycling on Li-ion Batteries (2025), © the authors, CC BY 4.0. BatterMachine digitized experimental markers in figures 4b, 4d and 5c, converted units and rounded the results. The released browser model is BatterMachine’s independent fit. Publication · Data license
UPV pouch temperature field
The original finite-volume heat solver advances 855 volumes over the measured 87 × 187 × 11 mm pouch, using direction-dependent conductivity. Two regions of one face set the effective heat-source coefficients using measurements from 5 to 210 s. The opposite-face temperatures were held out. At 480 s under the 35 A reference protocol, the lower sensor on that face measured 36.94 °C and the model gives 29.80 °C. The grid’s warmest volume reaches 30.69 °C. Probe coordinates inside the named regions are approximate. The interior field and its maximum have no independent interior measurement. Run the spatial model
Imad Elkourchi, Javier Marco-Gimeno, Carlos Micó and Antonio García, Universitat Politècnica de València. Experimental Dataset for Overcharge-Induced Thermal Runaway of a Semi-Solid-State Battery Cell and Mini-Module, with and without Active Liquid Cooling, Test 2, measurements of 13 June 2025. CC BY 4.0. BatterMachine aligned the Test 2 clock to the charger step, interpolated the measurements at five-second intervals and rounded them. Dataset and instrument description · Data license
Shen LFP electrical overcharge
Two full-charge 32 Ah prismatic LFP/graphite cells were overcharged under nominal 32 A and 40 A settings. Their one-second records include voltage, upper surface temperature and middle surface temperature. Delivered current and core temperature were unmeasured. The voltage channel can change its physical meaning when electrical contact changes. Missing values stay blank. Compare the experiments
Two empirical laws forecast the first voltage below 75% of its initial reading. One counts charge after subtracting a fitted constant current loss. The other combines terms proportional to current and current squared. The first observed voltage crossings at 16 A and 48 A set the coefficients. The 32 A and 40 A observations were reserved to test the forecasts. At 32 A the first recorded crossing is 829 s, compared with the forecasts of 849.9 s and 913.0 s. Temperature remains a measured time series. The voltage marker has no independent identification as the start of physical thermal runaway.
Jun Shen, overcharge-induced Thermal Runaway data in Prismatic Lithium Iron Phosphate Battery, Mendeley Data V1 (2025), CC BY 4.0. BatterMachine selected the 32 A and 40 A files, converted timestamps to elapsed seconds, and retained voltage and two of the recorded surface channels. Dataset · Data license · Experimental data credits